+高级检索
大尺寸无缝锆钛钢复合板的制备及性能
作者:
作者单位:

1.西安天力金属复合材料股份有限公司,陕西 西安 710201;2.西安理工大学,陕西 西安 710048;3.国家地方联合层状金属复合材料工程研究中心,陕西 西安 710201

作者简介:

通讯作者:

中图分类号:

基金项目:

Key R&D Plan of Shaanxi Province - Key project of two-chain integration(2021LLRH-05-09); Shaanxi Province Youth Talent Support Program Project(CLGC202234); Innovative pilot platform for layered metal composite materials (2024CX-GXPT-20)


Preparation and Performance of Large-Size Seamless Zirconium-Titanium-Steel Composite Plate
Author:
Affiliation:

1.Xi'an Tianli Clad Metal Materials Co., Ltd, Xi'an 710201, China;2.Xi'an University of Technology, Xi'an 710048, China;3.National Local Joint Layered Metal Composite Materials Engineering Research Center, Xi 'an 710201, China

Fund Project:

Key RD Plan of Shaanxi Province (2021LLRH-05-09); Shaanxi Province Youth Talent Support Program Project (CLGC202234); Sponsored by Innovative Pilot Platform for Layered Metal Composite Materials (2024CX-GXPT-20)

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    采用爆炸焊接+轧制法制备尺寸为2500 mm×7800 mm×(3+0.7+22) mm的锆钛钢复合板,并通过超声波无损检测、相控阵波形形貌、界面结构形状、电子扫描和力学性能测试对其性能进行了分析。结果表明:锆钛复合体的轧制温度应该控制在760 ℃,道次的压下量应控制在10%~25%。制备锆钛钢复合板的爆炸速度应控制在2450~2500 m/s,密度应为0.78 g/cm3,间隙高度应为12 mm,A区和B区的炸药高度为45~50 mm。爆炸焊接+轧制技术减少了爆炸焊接的冲击和多次热处理对材料性能的影响,同时解决了大尺寸锆钛钢复合板制备过程中出现的表面褶皱和开裂问题。

    Abstract:

    Zirconium-titanium-steel composite plate with the size of 2500 mm×7800 mm×(3+0.7+22) mm was prepared by explosive welding+rolling method, and its properties were analyzed by ultrasonic nondestructive testing, phased array waveform shape, interface structure shape, electronic scanning, and mechanical property testing. Results show that the rolling temperature of zirconium-titanium complex should be controlled at 760 °C, and the rolling reduction of each pass should be controlled at 10%–25%. The explosive velocity to prepare zirconium-titanium-steel composite plates should be controlled at 2450–2500 m/s, the density should be 0.78 g/cm3, the stand-off height should be 12 mm, and the explosive height of Zone A and Zone B should be 45–50 mm. Explosive welding combined with rolling method reduces the impact of explosive welding and multiple heat treatment on material properties. Meanwhile, the problems of surface wrinkling and cracking, which occur during the preparation process of large-sized zirconium-titanium-steel composite plate, can be solved.

    参考文献
    相似文献
    引证文献
引用本文

吴江涛,王丁,黄杏利,邹军涛,张鹏辉,高瑞博,杨欢,张涛,任倩玉,魏永.大尺寸无缝锆钛钢复合板的制备及性能[J].稀有金属材料与工程,2025,54(2):319~326.[Wu Jiangtao, Wang Ding, Huang Xingli, Zou Juntao, Zhang Penghui, Gao Ruibo, Yang Huan, Zhang Tao, Ren Qianyu, Wei Yong. Preparation and Performance of Large-Size Seamless Zirconium-Titanium-Steel Composite Plate[J]. Rare Metal Materials and Engineering,2025,54(2):319~326.]
DOI:10.12442/j. issn.1002-185X.20240438

复制
文章指标
  • 点击次数:
  • 下载次数:
  • HTML阅读次数:
  • 引用次数:
历史
  • 收稿日期:2024-07-18
  • 最后修改日期:2024-09-29
  • 录用日期:2024-10-12
  • 在线发布日期: 2025-02-25
  • 出版日期: 2025-02-20